Heat shrink sleeve peel test.

Heat shrink sleeve peel test.

I share a summary of the adhesion test method used on shrink sleeves.

The proyect was an aqueduct with  48-inch nominal diameter with 3LPE external coating and heat shrink sleeves in the welded joints.

For this evaluation we use ASTM D3330, method F: single layer tapes, peeled at 90 °.
No hay texto alternativo para esta imagen
Procedure:

·      Cut a rectangle 25 cm wide by 12 cm long with a knife

·      For 60 seconds we apply a constant force of at least 7.8?????? / ???? at 90 ° peel.

·      Evaluate the failure mechanism

Cohesive failure 

Adhesive failure

No hay texto alternativo para esta imagen
I share it hoping it will be of interest to you



Pedro Dávila Zú?iga

AMPP Coating Inspector Level 2

3 个月

A qué velocidad realizaste el ensayo

回复

Please can you provide the list of equipment/instruments used to carry out the peel test. Most especially the metal used to clip the strip of coating (peeled coating)

回复
Engr Sher Zaman

Assistant Manager Cathodic Protection Services at Bureau Veritas Group

3 年

7.5 or 78 Kgf/in What is f in the unit

回复
Engr Sher Zaman

Assistant Manager Cathodic Protection Services at Bureau Veritas Group

3 年

Minimum how much force should have for peel test

回复

要查看或添加评论,请登录

Diego Erazo的更多文章

社区洞察

其他会员也浏览了